QLQ zinc alloy surface finishing equipment and process QLQ zinc alloy surface finishing equipment and process

Professional Zinc Alloy Surface Finishing Solutions

Speical color

Speical color

1. Process Flow Chart

Speical color - image 1

2. Process Video

3. Process Details

After preprocessing and nickel plating, the next step is:

1. Oil removal electrolysis

1. Oil removal electrolysis

2. Three times Cleaning Tank

2. Three times Cleaning Tank

Remove residual liquid on the workpiece surface.

3. Dull nickel for 1 minute

Removing the brightness of nickel

4. Three times Cleaning Tank

4. Three times Cleaning Tank

Remove residual liquid on the workpiece surface.

5. Chromium plating

6. Two-grid recovery tank

6. Two-grid recovery tank

7. Six times Cleaning Tank

7. Six times Cleaning Tank

Remove residual liquid on the workpiece surface.

Get a Free Quote Today

Send us your samples or drawings — our engineers reply within 24 hours with pricing and technical advice.

Contact Us
Workshop Planning Data

Speical color — Data Zinc Alloy Finishing Managers Need

The rack plating line handles larger zinc alloy parts, sliders on frames and parts requiring precise current distribution — high-end finishes with zero contact marks and excellent throwing power.

800 m²Workshop Area
26 peopleTeam Size
330 kWInstalled Power
300-600k pcs/dayDaily Output (10 h)

Quality Inspection & Control

Check itemMethodAcceptance standard
Coating thicknessX-ray / coulometricCu 5-12 μm, Ni 5-15 μm per spec
AdhesionBend + thermal shockNo blister at 150 °C × 30 min
Color & glossColorimeter / gloss meterΔE ≤ 1.0, gloss per customer card
Contact marksVisual 10×Zero rack contact marks on A-surface
Salt sprayNSS chamber12-96 h per spec
Throwing powerCross-section microMinimum:maximum thickness ≥ 1:1.6

Workshop Layout & Floor Area

ZoneArea
Rack line (16-20 tanks)320 m²
Rack loading / unloading90 m²
Rectifier & control room50 m²
QA lab + microscope60 m²
Rack maintenance60 m²
Chemical store60 m²
Waste treatment120 m²
Utility & lockers40 m²
Total workshop800 m²

Manpower & Shift Plan

RoleHeadcount
Rack loaders / operators12
Chemical technicians3
QC inspectors3
Rack maintenance2
Wastewater operator1
Supervisor1
Maintenance / electrician2
Logistics2
Total (2 shifts × 10 h)26

Power & Utility Demand

EquipmentDemand
Rectifiers 0-15 V × 1000-3000 A120 kW
Tank heating / cooling70 kW
Hoist / transporter system30 kW
Pumps / filters / dosing38 kW
Exhaust + scrubber25 kW
Dryer / oven22 kW
Wastewater treatment20 kW
Lighting & auxiliary5 kW
Installed total330 kW
Typical running load≈ 260 kW

Production Flow Chart

PretreatmentHand / barrel polish, degrease
Rack LoadingLoad parts on plated copper racks
Copper Strike & BuildAlkaline Cu → acid Cu
Nickel / Color PlatingBright Ni, gold, gun, black etc.
Rinse ChainRecovery → DI rinse
Dry / Unload / QCOven dry, unload, inspect, pack

Daily Capacity — 10-Hour Operating Day

ParameterValue
Cycle per flight bar35-60 min
Parts per flight bar3,000-8,000
Flight bars per 10 h day14-18
Daily output300,000-600,000 pcs
Monthly output (26 days)8-15 million pcs

Output Value Estimate

ParameterValue
Plating fee per pieceUSD 0.015-0.04
Daily output value (10 h)USD 8,000-18,000
Monthly output valueUSD 210,000-470,000
Annual output valueUSD 2,500,000-5,600,000

Related Products — Complete Speical color Solution

Machines, chemicals and consumables selected from the real QLQ product range for this process. Every product page is live and ready to quote.

View Full Product Range

Special colour control points

Target colourBase layerTop processMain risk
Rose goldBright nickel or copperGold alloy bath, short dwellPink shift with copper content
BlackNickelBlack chrome or black nickelPurple haze under strong light
GunmetalNickelDark alloy or dyed sealBatch-to-batch lightness drift
Two-toneNickelPlate + mask + second plateMask leakage on relief edges

FAQ

Why does rose gold look different on brass and on zinc alloy?

Different base colour and surface finish. Fix the base spec first, then tune the bath.

How do we control two-tone registration?

Fixture design and mask thickness. Inspect the first part of every rack, not the last.

What light should colour be approved under?

D65 daylight, on a neutral grey background, with the approved chip beside the part.

FAQ

What about speical color — data zinc alloy finishing managers need?
The rack plating line handles larger zinc alloy parts, sliders on frames and parts requiring precise current distribution — high-end finishes with zero contact marks and excellent throwing power. 800 m² Workshop Area 26 people Team Size 330 kW Installed Power 300-600k pcs/day Daily Output (10 h)
What about quality inspection & control?
Check item Method Acceptance standard Coating thickness X-ray / coulometric Cu 5-12 μm, Ni 5-15 μm per spec Adhesion Bend + thermal shock No blister at 150 °C × 30 min Color & gloss Colorimeter / gloss meter ΔE ≤ 1.0, gloss per customer card Contact marks Visual 10× Zero rack contact marks on A-surface Salt spray NSS c
What about workshop layout & floor area?
Zone Area Rack line (16-20 tanks) 320 m² Rack loading / unloading 90 m² Rectifier & control room 50 m² QA lab + microscope 60 m² Rack maintenance 60 m² Chemical store 60 m² Waste treatment 120 m² Utility & lockers 40 m² Total workshop 800 m²
What about manpower & shift plan?
Role Headcount Rack loaders / operators 12 Chemical technicians 3 QC inspectors 3 Rack maintenance 2 Wastewater operator 1 Supervisor 1 Maintenance / electrician 2 Logistics 2 Total (2 shifts × 10 h) 26