Triage: symptom → confirm → first move

SymptomLikely rootConfirm byFirst move
Film wipes off, powderyBath too hot / too longTime-temperature logCut dwell; check heater
Iridescent patchy colorsUneven zinc surface from rinse dragPre-chromate rinse checkFix counter-flow rinse
Bare spots after chromateOil/silicone on zincWater-break test before chromatePre-clean audit
Weak color, fades fastBath exhausted / pH driftTitration + pHRebalance per TDS
Color varies by rack rowDrag-in concentration gradientPosition samplingDip discipline; agitation

Engineer notes

  • One variable per corrective action; verify with the confirm-by column.
  • Records beat memory: log every trial on the tank card.
  • Two failed actions in a row is a senior call — escalate with your log.
Safety: hexavalent chromate is a known carcinogen and sensitizer. Gloves, apron, face shield, exhaust on; trivalent lines preferred wherever spec allows.

FAQ

Patchy iridescence — bath or rinse?
Rinse first: drag-in contaminating the film shows as patches; check the pre-chromate rinse.
How do I time trivalent vs hexavalent?
Trivalent 30–90 s, hexavalent 15–45 s by color target — set a timer, not a habit.
Why does color drift through the shift?
Drag-in concentrates the bath and pH drifts; titrate and log.
Previous Post
Zinc Chromate Film Failure: The fix set with windows | Pre-treatment & Cleaning Senior Guide
Next Post
Zinc Chromate Film Failure: Recognise, record, escalate | Pre-treatment & Cleaning Junior Guide