Process: Rack Plating. Figures in this guide are industry-standard starting ranges; confirm against your supplier TDS before locking settings.

Working ranges and control points

The table below is the daily reference for a plating line. Set by the card, verify by the control point column.

ParameterTypical rangeControl pointWatch out
Contact point size0.5–2 mm² wire wrapMark hidden in seal areaMarks on visible faces
Rack angle10–20° from verticalSolution drains offAir pockets in cavities
Current density1–6 A/dm² by bathPer-position amp mappingHigh spots burn first
Auxiliary anode gap20–50 mmUniform throw into recessToo close plates dendrites
Load weightPer rack card limitWeigh-in random checkOverload sags contacts

Standard routine

  1. Read the rack card for current and position map
  2. Wrap contacts to hide marks in sealed zones
  3. Set angle so cavities drain
  4. Confirm auxiliary anodes are on before load-in
  5. Check first article thickness at three positions
Rack Plating junior - Live line operation - QLQ workshop photo
Live line operation — QLQ workshop photo

Engineer notes

  • The first article after every rack repair gets three-point thickness check
  • High-current corners need thieves or shields, not lower total amps
  • Bent racks plate bent parts — straighten on the bench, not in the tank
  • Log which rack frames run which part families to trace marks
  • Insulate worn tape spots before they plate over
Safety: Racks carry live current in the tank. Load and unload with the bus off; never touch two racks at once with bare hands.
Rack Plating junior - Close-up of the working zone - QLQ workshop photo
Close-up of the working zone — QLQ workshop photo

FAQ

Where should contact marks be placed?
On faces that get sealed, assembled or hidden — never on the show surface.
Why do recesses plate thin?
Throwing power limits current in cavities. Add auxiliary anodes or reduce total current and extend time.
How often are racks re-coated?
When insulation chips expose metal outside contact zones — usually every 3–6 months.