Barrel Plating Technician - Intermediate

Barrel Marks And Cat-Eye Defects: Triage: symptom → confirm → first move | Barrel Plating Intermediate Guide

Scope of this guide

Intermediate version: symptom-to-cause triage with the confirm-by column — find the variable, run one change, verify.

Series: finishing.com recurring questions answered with platingclub line practice. Parameters are industry-standard starting ranges — confirm against your supplier TDS.

Triage: symptom → confirm → first move

SymptomLikely rootConfirm byFirst move
Shiny oval spot on one faceContact mark from dangler/doorFace map vs barrel contact pointsRotate parts; pad door contact
Bare kidney-shaped patchParts nested face-to-faceNested pair in load sampleMedia ratio up; load size down
Line across several partsBarrel door edge rubbingTrack along door lineDoor liner check
Ring at part edgeMedia imprintMedia type checkChange media size/hardness
Mark repeats every load, same partsPart geometry self-shadowsBy-part-family patternFamily-specific load card

Engineer notes

  • One variable per corrective action; verify with the confirm-by column.
  • Records beat memory: log every trial on the tank card.
  • Two failed actions in a row is a senior call — escalate with your log.
Safety: barrels pinch and loads are hot. Guards closed, hoist rated, heat gloves; lock-out before reaching anywhere near the door.

FAQ

Marks only on flat parts — why?
Nesting: flats stick face-to-face. Media ratio up, load size down.
How do I tell door marks from dangler marks?
Door marks line up along one line across parts; dangler marks sit at one point on one face.
When do I change media size?
When imprints show at edges or marks persist after loading fixes.
上一篇
Barrel Marks And Cat-Eye Defects: The fix set with windows | Barrel Plating Senior Guide
下一篇
Barrel Marks And Cat-Eye Defects: Recognise, record, escalate | Barrel Plating Junior Guide